How to Weld and Cut BRINAR® Wear-Resistant Steel
Welding BRINAR® wear-resistant steel requires preheat proportional to the carbon equivalent value (CEV) and plate thickness, low-hydrogen basic electrodes and interpass temperature control. BRINAR® CEV ranges from 0.41 (grade 400 at 15 mm) to 0.68 (grade 450 at 50 mm). Plasma and oxy-fuel cutting are feasible on all three grades.
General principles for welding wear-resistant steel
Wear-resistant steel is a quenched and tempered high-hardness steel. Welding introduces localised heat that can generate heat-affected zones (HAZ) with brittle microstructures if process variables are not controlled. The three key factors are: preheat, consumable selection and interpass temperature.
Carbon equivalent value (CEV) by grade and thickness
CEV is the main parameter for determining preheat requirements. BRINAR® values are:
| Grade | Thickness (mm) | CEV | CET |
|---|---|---|---|
| BRINAR® 400 | 15 | 0.41 | 0.28 |
| BRINAR® 400 | 40 | 0.45 | 0.30 |
| BRINAR® 400 | 100 | 0.68 | 0.41 |
| BRINAR® 450 | 15 | 0.48 | 0.35 |
| BRINAR® 450 | 50 | 0.68 | 0.41 |
| BRINAR® 500 | 40 | 0.66 | 0.44 |
Higher CEV means greater risk of hydrogen cracking in the HAZ and greater need for preheat.
Preheat
Preheat aims to reduce the cooling rate in the HAZ, decreasing the risk of brittle martensite formation and hydrogen cracking. General recommendations based on BRINAR® data are:
- BRINAR® 400, thin gauges (≤15 mm, CEV 0.41): Minimal or no preheat under controlled conditions (ambient temperature ≥10°C, low humidity).
- BRINAR® 400, medium gauges (40 mm, CEV 0.45): Preheat of 100–150°C recommended.
- BRINAR® 400, heavy gauges (100 mm, CEV 0.68): Preheat of 150–200°C required.
- BRINAR® 450 (CEV 0.48–0.68): Preheat of 125–175°C depending on thickness.
- BRINAR® 500 (CEV 0.66): Preheat of 150–200°C required.
For specific welding procedure specification (WPS) parameters, consult the official Salzgitter technical documentation or contact the BRINAR® technical support team.
Electrode and consumable selection
Low-hydrogen basic electrodes are required for all BRINAR® grades. Diffusible hydrogen content must not exceed:
- BRINAR® 400 and 450: H ≤5 ml/100 g (H5 designation)
- BRINAR® 500: H ≤2 ml/100 g (H2 designation) — the lowest available level is recommended
Consumables should have a tensile strength lower than that of the base metal to concentrate plastic deformation in the weld bead rather than in the HAZ.
Interpass temperature
Maximum interpass temperature must be controlled to avoid excessive softening of the HAZ. As a general rule, the tempering temperature of the base steel should not be exceeded. Heating during machining of BRINAR® must not exceed 175°C to preserve mechanical properties.
Plasma cutting and oxy-fuel cutting
Both plasma cutting and oxy-fuel cutting are feasible for all three BRINAR® grades. Plasma cutting is preferred due to its lower heat input and smaller HAZ. For oxy-fuel cutting on heavy gauges, preheating the cutting zone is recommended, especially for BRINAR® 500, to avoid edge cracking.
Laser cutting is also an efficient option for thin and medium gauges, offering the smallest HAZ of the three methods.
Post-weld heat treatment
For BRINAR® 400 and 450, post-weld heat treatment (PWHT) is generally not required for moderate thicknesses. For BRINAR® 500 and heavy gauges of any grade, a stress-relief PWHT may be beneficial, but must be performed at a temperature below the original tempering temperature of the steel.
General recommendations
- Store electrodes in holding ovens at the temperature indicated by the manufacturer.
- Clean the joint by removing rust, paint, grease and moisture before welding.
- Avoid rapid cooling — allow slow cooling under a thermal blanket if necessary.
- Check hardness in the HAZ after welding to confirm that excessive softening has not occurred.
- Document the welding procedure and maintain it as a qualified WPS for each application.
Frequently asked questions
What type of electrode is recommended for welding wear-resistant steel?
Low-hydrogen basic electrodes are recommended. For BRINAR® 400 and 450, diffusible hydrogen content must not exceed 5 ml/100 g (H5). For BRINAR® 500, a maximum of 2 ml/100 g (H2) is required. Consumables should have lower strength than the base metal.
Is preheating necessary before welding BRINAR® 400?
It depends on the thickness. At thin gauges (≤15 mm) with a CEV of 0.41, preheat can be minimal under controlled conditions. At 40 mm thickness (CEV 0.45), 100–150°C is recommended, and at 100 mm (CEV 0.68), 150–200°C is required.
Can wear-resistant steel be cut with plasma?
Yes, plasma cutting is feasible and preferred for all three BRINAR® grades due to its lower heat input and smaller heat-affected zone (HAZ). Oxy-fuel cutting is also feasible, although for heavy gauges of BRINAR® 500, preheating the cutting zone is recommended.
What is the maximum interpass temperature when welding wear-resistant steel?
Interpass temperature must not exceed the tempering temperature of the base steel. For BRINAR®, heating during machining must not exceed 175°C to preserve mechanical properties. Consult the official Salzgitter documentation for specific parameters for each grade and thickness.
Related grades
Need wear-resistant steel for your project?
Quote BRINAR® 400, 450 or 500 with delivery from our warehouse in Monterrey.