AR400 vs AR450 vs AR500: Complete Wear-Resistant Steel Comparison

AR400, AR450 and AR500 wear-resistant steels differ primarily in their Brinell hardness: 370-440 HB, 420-470 HB and 470-540 HB respectively. Higher hardness means greater abrasion resistance but lower toughness and weldability. AR400 is ideal for applications with moderate impact, AR450 for severe wear with limited impact, and AR500 for extreme abrasion with very hard minerals.

AR400 vs AR450 vs AR500 comparison summary

Choosing the right wear-resistant steel grade is a critical decision that directly impacts component service life, total cost of ownership and ease of fabrication. BRINAR® offers three main grades — 400, 450 and 500 — each optimised for a distinct range of working conditions. This guide compares their mechanical, chemical and processing properties to help you select the right grade.

Mechanical properties comparison table

PropertyBRINAR® 400BRINAR® 450BRINAR® 500
Material no.1.87141.87221.8734
Hardness (HB)370–440420–470470–540
Yield point (MPa)9601,1001,300
Tensile strength (MPa)1,2001,3501,500
Elongation at rupture (%)1297
Impact energy at −20°C (J)604030
Maximum thickness (mm)12010080

Brinell hardness and wear resistance

Brinell hardness is the most direct indicator of abrasion resistance. BRINAR® 400 guarantees a range of 370–440 HB, while BRINAR® 450 rises to 420–470 HB and BRINAR® 500 reaches 470–540 HB. In practical terms, each grade increment can represent 15% to 50% longer service life against pure sliding abrasion, depending on the mineral and operating conditions.

Toughness and impact resistance

Toughness decreases as hardness increases. BRINAR® 400 offers 60 J of Charpy impact energy at −20°C, making it the best choice when significant impact loads are present (shovel buckets, dump truck bodies with coarse material). BRINAR® 450 offers 40 J, suitable for moderate impacts. BRINAR® 500 has 30 J, recommended only when abrasion dominates and impact is low.

Elongation follows the same trend: 12% (400), 9% (450) and 7% (500). Higher elongation means greater deformation capacity before fracture, which is critical in components subjected to dynamic loads.

Weldability

Weldability is directly linked to the carbon equivalent value (CEV). BRINAR® 400 has a CEV of 0.41 at 15 mm thickness, allowing welding with minimal preheat. BRINAR® 450 has a CEV of 0.48 at 15 mm, requiring preheat between 125°C and 175°C. BRINAR® 500, with a CEV of 0.66 at 40 mm, demands preheat of 150–200°C and very low-hydrogen basic electrodes.

In all cases, the use of low-hydrogen basic electrodes and strict interpass temperature control is recommended.

Available thicknesses

BRINAR® 400 is available up to 120 mm, offering the greatest versatility in heavy gauges. BRINAR® 450 reaches up to 100 mm and BRINAR® 500 up to 80 mm. This difference is relevant in applications requiring thick sections, such as crusher liners or large-capacity hoppers.

When to use each grade

  • BRINAR® 400: Applications with moderate to severe impact combined with wear: mining buckets, dump truck bodies, mineral transport chutes, earthmoving equipment.
  • BRINAR® 450: Severe wear with limited impact: crusher liners, conveyor belt wear plates, high-tonnage excavator buckets.
  • BRINAR® 500: Extreme abrasion with very hard minerals (silica, basalt, granite) and low impact: bucket teeth and lips, mill liners, coke and slag gates.

Chemical composition comparison

All three grades share a similar chemical base with Cr, Mo, Ni and B as the main alloying elements. The key differences are:

ElementBRINAR® 400 (max %)BRINAR® 450 (max %)BRINAR® 500 (max %)
C0.300.260.32
Si0.600.600.80
Mn1.501.501.50
Cr1.801.801.80
Mo0.600.650.65
Ni2.102.102.10

Conclusion

There is no universal grade. Selection should be based on the predominant type of wear (abrasion vs impact), required thickness and fabrication needs (weldability, bending). When abrasion dominates, choose the hardest grade your fabrication process allows. When impact is significant, prioritise the toughness of BRINAR® 400.

Frequently asked questions

What is the main difference between AR400, AR450 and AR500?

The main difference is Brinell hardness: AR400 offers 370–440 HB, AR450 offers 420–470 HB and AR500 offers 470–540 HB. Higher hardness means greater abrasion resistance but lower impact toughness and lower elongation.

Which wear-resistant steel grade is best for dump truck bodies?

For dump truck bodies, BRINAR® 400 is the most common choice due to its balance between wear resistance and impact toughness (60 J at −20°C). In operations with extremely abrasive material and low impact, BRINAR® 450 may offer longer service life.

Can AR500 wear-resistant steel be welded?

Yes, BRINAR® 500 can be welded, but requires special precautions: preheat of 150–200°C, very low-hydrogen basic electrodes and strict interpass temperature control. Its CEV of 0.66 (at 40 mm) demands a qualified welding procedure.

How much longer does an AR500 plate last compared to AR400?

Under pure sliding abrasion conditions, BRINAR® 500 can offer 30% to 50% longer service life than BRINAR® 400. However, in applications with significant impact, the higher toughness of BRINAR® 400 may result in superior service life by avoiding brittle fracture.

Related grades

Need wear-resistant steel for your project?

Quote BRINAR® 400, 450 or 500 with delivery from our warehouse in Monterrey.